Sheet Metal Bend Radius Chart by Material and Thickness

Mandeep
November 10, 2026

In this note

A fabricator once called me about a drawing of ours that had R 0.5 on a 3 mm 6061 T6 bracket, and he asked, politely, whether we wanted the parts cracked or made to a radius the material could actually take. I was heading supply chain at the time, the drawing had been through our engineering review, and nobody had picked that radius, the CAD default had. That call taught me the thing about a sheet metal bend radius that I now explain to buyers every week, the material picks it before you do, and the drawings that cause trouble are the ones where a designer or a default picked it instead. This page is the sheet metal bend radius chart I wish someone had handed me that week, minimum inside radius by material and thickness, then the K factor, bend allowance and bend deduction worked on one plain bend, and the 3 rules about flanges, holes and grain that keep a bent part out of the scrap bin.

Let's start with why the material picks the radius before you do

Fold a 2 mm steel sheet to 90 degrees and 3 things happen at once. The outside of the bend stretches, the inside compresses, and somewhere between them a line called the neutral axis keeps its length. The tighter the inside radius, the more the outside has to stretch, and every material has a stretch it cannot exceed before it cracks, which is the elongation figure on its mill certificate. That is the whole physics, and it is why the chart below is really a list of how far each coil can stretch.

Soft, ductile coils like annealed brass and 3003 aluminum stretch a long way and bend almost to nothing, and the Aluminum Association publishes bend data for every temper. Cold rolled steel and annealed 304 stainless bend to about their own thickness. High strength steels and 6061 T6 aluminum, which traded ductility for strength, need 2 to 3 times their thickness or they split on the outside of the bend, which is exactly what that fabricator was trying to save us from. The plate below shows the bend in section, and then comes the chart.

The chart, minimum inside bend radius by material and thickness

Minimum inside radius for a 90 degree bend across the grain, in the tempers a stamping or fabrication plant normally buys, given first as a multiple of thickness and then in millimetres for 3 common gauges. These are typical production minimums, not the absolute limit a lab can reach, and the drawing and the coil certificate govern. If you want the sheet metal bend radius chart pdf to pin above a desk, ask and we will send it.

Material and temperMinimum R, times TR at 1.5 mmR at 3.0 mmR at 6.0 mm
Cold rolled steel, 1008 to 1010, ASTM A10081 t, 0.5 t possible1.53.06.0
Hot rolled pickled and oiled, ASTM A10111 to 1.5 t1.5 to 2.33.0 to 4.56.0 to 9.0
HSLA grade 50, ASTM A10111.5 to 2 t2.3 to 3.04.5 to 6.09.0 to 12.0
HSLA grade 80, ASTM A10112.5 to 3 t3.8 to 4.57.5 to 9.015 to 18
Stainless 304, annealed1 t, 0.5 t possible1.53.06.0
Stainless 301, half hard2 t3.06.0not stocked
Stainless 430, annealed1 t1.53.06.0
Aluminum 3003 H140.5 t0.81.53.0
Aluminum 5052 H321 t, 1.5 t over 3 mm1.53.09.0
Aluminum 6061 T62.5 to 3 t3.8 to 4.57.5 to 9.015 to 18
Aluminum 6061 O or T4, aged after forming1 t1.53.06.0
Brass C260, annealed0 to 0.5 t0 to 0.80 to 1.50 to 3.0
Copper C110, annealed0.5 t0.81.53.0
Galvanized G90, ASTM A6531 t1.53.06.0

Our 6061 T6 bracket is the third row from the bottom, and at 3 mm it wanted 7.5 to 9 mm of inside radius, not 0.5. We redrew it at R 8 where the radius did not matter, and on the one flange where it did we switched the part to 5052 H32 and got R 3, which is the kind of swap the chart makes obvious once it is in front of you.

Why the chart is a minimum, and what the press brake actually makes

The chart gives the smallest radius the material survives, and a press brake rarely makes exactly that number, because in air bending the inside radius is set by the V opening of the die, not by the punch tip. A plant bends 2 mm steel in a V of about 12 to 16 mm, 6 to 8 times thickness, and the radius that forms is roughly a sixth of the V, so about 2 to 2.7 mm, which is comfortably above the 1 t minimum and is what the part will have whatever the drawing says.

Write R 1.0 on a 2 mm steel part and the plant will either bottom the bend in a tighter die at a higher price or, more often, make it at R 2 and nobody will notice. Write R 2.0 or R 2.5 and the drawing matches the press. In a stamping die the radius is machined into the form steel, so the die holds what the drawing says, down to the chart minimum, and tighter than the chart means cracked parts from the first hit, so either way the chart number is the floor, and your drawing should sit on it or above it. The radius also decides how long the flat blank has to be, which is the next piece of math.

Air bending a steel bracket on a CNC press brake at a partner facility in India
Air bending on the press brake at one of our manufacturing partners, where the V opening sets the radius, the back stop sets the flange, and the punch only pushes

Let's work one bend, K factor, bend allowance and the flat pattern

The flat blank is shorter than the sum of the bent legs, because the outside of the bend stretched, and the number that corrects for it comes from the neutral axis in the plate above. The K factor is where that axis sits, as a fraction of thickness measured from the inside of the bend, and for air bent steel at about 1 t radius it is close to 0.42, dropping toward 0.33 on very tight bends and rising toward 0.5 on radii much larger than the thickness. Take the plate, 2 mm cold rolled steel, 90 degrees, inside radius 2 mm, K 0.42, and here is the math.

  1. Bend allowance, the length of the neutral axis through the bend, is π ÷ 180 × 90 × (R + K × T), which is 1.5708 × 2.84, or 4.46 mm.
  2. Setback from the outside corner to the start of the bend is (R + T) × tan 45°, which is 4.00 × 1, or 4.00 mm.
  3. Bend deduction is twice the setback minus the bend allowance, 8.00 minus 4.46, or 3.54 mm.
  4. If the 2 legs measure 50 and 30 mm to the outside, the flat blank is 80 minus 3.54, which is 76.46 mm.

Every CAD package does this for you, and every CAD package uses a default K factor that may not be the plant’s, which is why the plant’s first article report shows the flat it actually cut, and why a flange that comes out 0.3 mm short is usually a K factor and not a press brake operator. The sheet metal tolerance note covers what a formed dimension holds once the bend is in. Three more rules sit near every bend, and they are about distance.

The three dimensions that live near a bend

Three rules keep a bent part out of trouble, and all 3 are about distance from the bend. The minimum flange, measured to the outside, is about 4 times the thickness plus the radius, because a shorter leg falls into the V and never forms, so on 2 mm steel at R 2 that is 10 mm, and a 7 mm flange on that drawing will come back with a question. A hole should sit at least 2.5 times thickness plus the radius from the bend line, 7 mm on the same part, or the bend pulls it oval and the die or the brake marks it, and if the design needs it closer, the hole is pierced after bending at a cost.

A bend that stops partway along an edge needs a relief cut at its end, a slot about the thickness wide and the radius plus thickness deep, or the material tears at the corner where the bent and flat parts meet. None of these are tolerances, they are geometry, and they sit alongside the general tolerance on the drawing, so a flange at 10 mm nominal and ±0.3 can still be 9.7 and still be a good part, which our manufacturing partners will confirm on the DFM call. The last 2 things the chart does not show are grain and springback, and they are behind the 2 cracks I still see.

Bent steel brackets at first article inspection on the bench at a partner facility in India
Bent bracket at first article at one of our manufacturing partners, where flange length, hole to bend and the relief at the corner are the 3 checks on the sheet

Grain, springback, and the two cracks I still see on first articles

Coil has a grain from the rolling mill, and a bend made along the grain cracks at a radius that the same bend across the grain takes easily, so a plant lays the blank out with critical bends across the grain, and a part with bends in both directions on a tight radius needs the radius opened on one of them, about 50 percent larger along the grain as a working rule. Springback is the other thing the chart does not show, because steel opens 1 to 3 degrees after the punch lifts, HSLA and aluminum 3 to 6, and the press brake operator overbends to compensate, part by part on a CNC brake and once in the die on a stamping.

The 2 cracks I still see on first articles, after all these years, are 6061 T6 bent to the 5052 radius on a drawing that said aluminum and nothing else, and HSLA bent on a die designed for cold rolled steel at 1 t. Both are the material line on the drawing doing the damage, not the press, and both are caught in the first 5 minutes of a DFM review if the material and temper are written down.

Our engineers are in the partner press shops and fabrication plants every day, not on visits, so that review happens with the drawing and the coil certificate side by side, and the weekly tollgate email you get every Friday lists every open item, the date it was promised and the date it will land.

I spent 13 years signing drawings before a fabricator was kind enough to make that call, and I would rather you did not wait that long. If you have a bent part on your desk and you are not sure the radius is one the material will take, send it over with the material and thickness, and we will return it with every bend checked against this chart and the V the plant will use, inside 48 hours.

What engineers ask about sheet metal bend radius

What is the standard sheet metal bend radius?

For cold rolled steel, annealed 304 stainless and 5052 H32 aluminum, an inside radius equal to the sheet thickness is the standard sheet metal bend radius a plant works to. Softer coils such as 3003 aluminum and annealed brass bend tighter, and HSLA and 6061 T6 need 1.5 to 3 times thickness.

What is the minimum bend radius for aluminum sheet?

3003 H14 bends to about half its thickness, 5052 H32 to about one times thickness up to 3 mm and 1.5 times above, and 6061 T6 needs 2.5 to 3 times thickness or it cracks on the outside of the bend. Forming 6061 in the O or T4 condition and ageing afterwards brings it back to about one times thickness.

How do I calculate bend allowance?

Bend allowance equals π ÷ 180 × the bend angle × (inside radius + K factor × thickness). For 2 mm steel at 90 degrees, R 2 and K 0.42, that is 1.5708 × 2.84, or 4.46 mm, and the bend deduction is twice the setback minus that, 3.54 mm, so the flat blank is the sum of the outside legs minus 3.54 mm.

What K factor should I use?

About 0.42 for air bent steel at a radius near one times thickness, dropping toward 0.33 on very tight bends and rising toward 0.5 when the radius is much larger than the thickness. Ask the plant for the K factor it uses, because a CAD default that differs from the plant is the usual reason a flange comes out 0.3 mm short.

Send your drawing.Full landed cost in 5 business days.

DFM notes inside 48 hours. Part price, tooling, freight and duty shown as separate lines. First response inside 24 hours.

Send RFQ now
Mandeep Singh, Co-Founder and CEO of VIA INDIGOS, who writes and reviews the From the floor notes
Reviewed by Mandeep Singh, Co-Founder and CEO, VIA INDIGOS 13+ years buying engineered parts before founding VIA INDIGOS.

This website stores cookies on your computer. Cookie Policy